Abstract:
Sm (Co
balFe
0.1Cu
0.1Zr
0.033)
7.5permanent magnets was prepared by powder metallurgy method with an addition of liquid phase La
3Co.The effects of La
3Co addition on the demagnetization curve, remanence, coercivity and mechanism of high temperature coercivity of Sm (Co
balFe
0.1Cu
0.1Zr
0.033)
7.5permanent magnets were studied.It was found that demagnetization curve was improved with La
3Co addition, due to the change of cell structure in the magnets.As the addition of La
3Co comes to 3%, the magnet achieves the best demagnetization curve, while as the addition of La
3Co comes to 5%, the demagnetization curve becomes deviation again.Remanence and magnetic energy product, which are intrinsic magnetic properties for the magnetic materials, decreased with La
3Co addition account to the La element is a non-magnetic element.The coercivity at room temperature decreased with the addition of La
3Co increasing, which account to the 1:5 cell boundary phase volume fractions increase.Coercivity mechanism of the precipitation-hardened Sm (Co
balFe
0.1Cu
0.1Zr
0.033)
7.5high-temperature magnets was described by the theory of single-phase permanent magnets.The addition of La
3Co reduce the exchange coupling between the cell body and improve the coercivity in high temperature of permanent magnet, when the addition of La
3Co come to 3%, the coercivity of the magnets at high temperature 500℃reaches 0.9T.